Drilling

Drilling stainless steel without work-hardening the hole

Austenitic stainless hardens under a rubbing edge. Keep the feed positive, the coolant aimed, and never let a drill dwell in the cut.

6 min read

Why stainless punishes hesitation

Austenitic grades (304, 316, the ISO M group) work-harden when the cutting edge rubs instead of shears. A drill that dwells, a feed backed off to "protect" the tool, or a worn margin all leave a hardened skin that the next pass must cut through. The hole then fights every subsequent tool: reamers chatter, taps break, and the next drill wears in minutes.

The counter-intuitive rule is to feed harder, not softer. A positive feed per revolution keeps the edge under the hardened layer. For solid carbide drills in the SYIL SPO and LSMO series, start at the feed in the table below and reduce speed — not feed — when the machine complains.

Coolant is a chip-evacuation system, not a lubricant

In stainless, chips weld to the margin if they stay in the flute. Through-coolant drills (SPO-03/05/07 for steel and stainless, SNO for non-ferrous) push chips out ahead of the tool instead of dragging them up the bore. Filter to 20 µm or better and hold pressure at the values in the depth-ratio article linked below; emulsion at 8–10 % concentration is a reasonable starting point for M-group work.

Peck only when depth exceeds the series rating. Every retract in stainless is a chance to rub on re-entry; a correctly rated coolant-through drill should run the whole depth in one pass.

Starting values, Ø8 mm, emulsion 8 %

These are published starting points for SYIL solid carbide drills, not guarantees. Adjust from the first hole: listen, look at the chip colour, and measure the bore before changing two variables at once.

Material groupvc (m/min)f (mm/rev)SYIL series
ISO P, steel < 900 MPa90–1200.20–0.28SPO-03 / SPO-05
ISO M, stainless 304/31660–800.16–0.24SPO / LSMO deep-hole
ISO K, grey cast iron110–1500.25–0.35SKO-03 / SKO-05
ISO N, aluminium200–3000.25–0.40SNO-03 / SNO-05

When the hole is already hardened

If a previous tool left a glazed bore, do not send the same drill back in at the same parameters. Drop vc by a third, keep feed positive, and take the full diameter in one pass — a pilot hole in work-hardened stainless concentrates wear on the chisel edge. The XSP0-03 pilot drill exists for deep-hole starts in normal material, not for rescuing hardened ones.

Related tools