Implant-grade stainless: small deep holes without the hardened skin

316L work-hardens under a rubbing edge and galls on the margin. Coolant-through geometry, positive feed and one pass to depth.

Implant-grade stainless: small deep holes without the hardened skin
Insights - 12 Sep 2026

Why 316L is not 304 with a certificate

Implant and instrument work brings 316L and its cousins: lower carbon, more molybdenum, and a tendency to gall and work-harden that punishes any hesitation at the edge. The hole is often small and deep relative to diameter, and the surface finish is a functional requirement, not a cosmetic one - a hardened or torn bore fails passivation and fails inspection.

The rule set is the stainless rule set, tightened: positive feed per revolution, no dwell, no peck inside the series depth rating, and coolant aimed at the cutting edge rather than at the general area. SYIL SPO coolant-through drills and the LSMO deep-hole series carry the geometry for this; CMD micro drills cover the small-diameter end where margin width and point geometry decide whether the hole stays round.

One pass to depth, or not at all

Every retract in 316L is a re-entry through a work-hardened skin. A correctly rated coolant-through drill should run the whole depth in one pass at the feed in the table; if the depth exceeds the rating, change the series rather than pecking the short one. Filter coolant to 20 µm or better - a particle the size of the margin clearance is a scratch the length of the bore.

Hold concentration at 8-10 % for M-group work and watch chip colour: straw to light brown is healthy; blue chips and a singing margin mean speed is too high for the coolant you actually have, not the coolant you wish you had.

Diameter bandvc (m/min)f (mm/rev)SYIL series
Ø1-3 mm40-600.03-0.06CMD micro
Ø3-8 mm50-700.06-0.14SPO-03 / SPO-05
Ø8-12 mm, 5xD+50-700.12-0.20LSMO deep-hole
Pilot for hardened bore35-500.05-0.10XSP0 pilot

Finish is a process, not a pass

If the bore must be reamed or burnished after drilling, leave a uniform, small allowance and never send a worn drill back in to "clean it up". The hardened skin left by a rubbing drill concentrates wear on the next tool's chisel edge and prints a spiral the reamer cannot remove. The values above are published starting points for SYIL carbide, not guarantees; measure the first bore, look at the chip, and change one variable at a time.

In 316L every retract is a re-entry through hardened skin. One pass to depth, or change the series.